1. Material Requirements
Base material: 100% solid pine wood, no composite/engineered substitutes;
moisture content 8–12% (meets industry humidity standards).
No decay, insect infestation, or dead knots exceeding 5mm; live knots ≤15mm, spaced ≥100mm apart.
2. Finger Joint Quality
Joint structure: Interlocking finger profile with tight fit (gap ≤0.2mm);
adhesive: waterproof wood glue (meets EN 204 D3 standard).
Shear strength: ≥2.5N/mm² (tested via tensile shear test on random samples).
3. Dimensional & Flatness Tolerance
Thickness/width/length: ±0.5mm per meter (calibrated with digital caliper).
Flatness: ≤0.3mm/m (checked with straightedge and feeler gauge).
4. Appearance
Surface: Smooth, no splinters, cracks, or glue residue;
sanded to P240 or P180 grit (visual & tactile inspection).
Color: Uniform pine tone, no obvious discoloration or stains.
5. Inspection Methods
Sampling: 3% of each batch (min. 5 boards); full inspection for at least 80% batches (Nearly each units should be inspected).
Tools: Digital caliper, moisture meter, straightedge, feeler gauge, tensile tester.
Rejection: Any board failing 2+ criteria; re-inspect entire batch if 10%+ samples fail.
By Grace Xu from Cao County Huifengyuan Wooden Co., Ltd.